Eco-alloys
Chemical Composition
Wisco’s commercial reference | Elements | Alloys as per most current up to date specifications (% percentage values) | Closest International Standards |
| Cu | Sn | Pb | Zn | Ni | Σ Otros |
| W-5 E |
% min. % máx. |
81 87 |
Resto |
4,0 6,0 |
2,0 4,0 |
6,0 8,0 |
1,0 |
 |
| W-7 E |
% min. % máx. |
Resto |
Resto |
5,6 8 |
2,0 4,0 |
6,0 8,0 |
1,0 |
 |
Correlation of International Norms
- * As per European directive 2002/95/EC ROHS (Restriction Of Hazardous Substances)
- (2) Ni content considered as Cu.
- (5) Forgeable material and feasible for other additional processes after casting in order to improve mechanical characteristics; these final mechanical values will depend of the chosen process.
- (6) Excellent deformation in cold.
Mechanical Properties
Wisco’s commercial reference | Approximate Mechanical Characteristics at 20ºC. Minimum values |
Yield Point Rp 0.2N/mm² | Tensile Strength Rm N/mm² | Elongation A5 (%) | Hardness HB 10/100 | Yielding Module KN/mm² |
| W-5 E |
110 |
220 |
12 |
65 |
65 a 105 |
| W-7 E |
120 |
240 |
12 |
70 |
98 a 115 |
- * As per European directive 2002/95/EC ROHS (Restriction Of Hazardous Substances)
Physical Properties
Wisco’s commercial reference | Physical Properties |
Density Kg/dm² | Specific Heat j/g. k | Thermal Expansion 10-6 k | Thermal Conductivity W/m. º k | Electrical Conductivity m / (Ohm.mm²) |
| W-5 E |
8,8 |
0,373 |
18,2 |
71 |
8,5 |
| W-7 E |
8,8 |
0,356 |
18,5 |
64 |
8,5 |